A series of B-Ni2P/SBA-15/cord monolithic catalysts were prepared by coating the slurry of the B-Ni2P/SBA-15 precursors on a pretreated cordierite support, and followed by temperature-programmed reduction in a H2 flow...A series of B-Ni2P/SBA-15/cord monolithic catalysts were prepared by coating the slurry of the B-Ni2P/SBA-15 precursors on a pretreated cordierite support, and followed by temperature-programmed reduction in a H2 flow. The samples were characterized by X-ray diffraction (XRD) and N2 adsorption-desorption technique. The catalytic activities for the hydrodesulfurization (HDS) of dibenzothiophene (DBT) were evaluated. The results showed that Ni2P phase was present in all B-Ni2P/SBA-1 5/cord monolithic catalysts. The specific surface areas (SBET) of the B-Ni2P/SBA-15/cord monolithic catalysts was first increased to 167 m2· g-1, and then decreased to 155 m2· g-1 with the increase of boron contents. The catalytic activity also showed the similar trend with the increase of boron contents. The 1.75% (by mass) B-Ni2P/SBA-15/cord monolithic catalysts exhibited the highest DBT conversion of 98.4% at 380 ℃. The cordierite-based monolithic catalysts showed better low temperature sensitivity for HDS of DBT in comparison with the particle catalysts. Moreover, two HDS routes, direct desulfurization (DDS) and hydrogenation (HYD), proceeded independently over B-Ni2P/SBA-15/cord monolithic catalysts and the main pathway was DDS.展开更多
The Ni/Mo/SBA-15 catalyst was modified by La2O3 in order to improve its thermal stability and carbon deposition resistance during the CO2 reforming of methane to syngas. The catalytic performance, thermal stability, s...The Ni/Mo/SBA-15 catalyst was modified by La2O3 in order to improve its thermal stability and carbon deposition resistance during the CO2 reforming of methane to syngas. The catalytic performance, thermal stability, structure, dispersion of nickel and carbon deposition of the modified and unmodified catalysts were comparatively investigated by many characterization techniques such as N2 adsorption, H2-TPR, CO2-TPD, XRD, FT-IR and SEM. It was found that the major role of La2O3 additive was to improve the pore structure and inhibit carbon deposition on the catalyst surface. The La2O3 modified Ni/Mo/SBA-15 catalyst possessed a mesoporous structure and high surface area. The high surface area of the La2O3 modified catalysts resulted in strong interaction between Ni and Mo-La, which improved the dispersion of Ni, and retarded the sintering of Ni during the CO2 reforming process. The reaction evaluation results also showed that the La2O3 modified Ni/Mo/SBA-15 catalysts exhibited high stability.展开更多
基金Supported by the National Basic Research Program of China(2006CB202503)the Science Foundation of PetroChina(2010D-5006-0401)
摘要A series of B-Ni2P/SBA-15/cord monolithic catalysts were prepared by coating the slurry of the B-Ni2P/SBA-15 precursors on a pretreated cordierite support, and followed by temperature-programmed reduction in a H2 flow. The samples were characterized by X-ray diffraction (XRD) and N2 adsorption-desorption technique. The catalytic activities for the hydrodesulfurization (HDS) of dibenzothiophene (DBT) were evaluated. The results showed that Ni2P phase was present in all B-Ni2P/SBA-1 5/cord monolithic catalysts. The specific surface areas (SBET) of the B-Ni2P/SBA-15/cord monolithic catalysts was first increased to 167 m2· g-1, and then decreased to 155 m2· g-1 with the increase of boron contents. The catalytic activity also showed the similar trend with the increase of boron contents. The 1.75% (by mass) B-Ni2P/SBA-15/cord monolithic catalysts exhibited the highest DBT conversion of 98.4% at 380 ℃. The cordierite-based monolithic catalysts showed better low temperature sensitivity for HDS of DBT in comparison with the particle catalysts. Moreover, two HDS routes, direct desulfurization (DDS) and hydrogenation (HYD), proceeded independently over B-Ni2P/SBA-15/cord monolithic catalysts and the main pathway was DDS.
基金supported by the Key Project of Chinese National Programs for Fundamental Research and Development(973 Program 2005CB221204)the Natural Science Fund of China(20676087)
摘要The Ni/Mo/SBA-15 catalyst was modified by La2O3 in order to improve its thermal stability and carbon deposition resistance during the CO2 reforming of methane to syngas. The catalytic performance, thermal stability, structure, dispersion of nickel and carbon deposition of the modified and unmodified catalysts were comparatively investigated by many characterization techniques such as N2 adsorption, H2-TPR, CO2-TPD, XRD, FT-IR and SEM. It was found that the major role of La2O3 additive was to improve the pore structure and inhibit carbon deposition on the catalyst surface. The La2O3 modified Ni/Mo/SBA-15 catalyst possessed a mesoporous structure and high surface area. The high surface area of the La2O3 modified catalysts resulted in strong interaction between Ni and Mo-La, which improved the dispersion of Ni, and retarded the sintering of Ni during the CO2 reforming process. The reaction evaluation results also showed that the La2O3 modified Ni/Mo/SBA-15 catalysts exhibited high stability.